Yep. I had one unspiral itself when I tried to drill with it. Thinking it was an isolated fault, I returned it to the supplier and the same thing happened with the replacement and with the replacement for the replacement, even though the supplier, a respected specialist supplier of drills to the engineering trade, assured me that they were all from different batches.

As I mostly use automatic machinery, I prefer solid carbide for stainless.

Colin Bignell

Yes, it works fine. Note the qualifier "old"

A lot depends on the hole size, and the rigidity of your drill press / hand drill.

If you try to drill 13mm straight off with a hand drill, then there's the potential for so a slight difference in cut depth from side to side turning into a considerable off-axis force. The hole is likely to wander like crazy, possibly with injury.

If you're drilling on a rigid drill press, then even then you can have problems with thin sheet (and I mean

When drilling thin stock, it's hard to beat a step drill. Makes a rounder hole (more round?) and is far less likely to snatch the material.

John

Better still to use a Q-Max type punch. Although IIRC 3 mm steel might be a bit much.

Just drilled to holes to mount my mill vise.

I used 450rpm.

First hole with a 1/8 drill.

Second hole with a 3/8 drill.

Steel plate thickness was 8mm.

my 2 cents

In article , Bruce Simpson writes

Not really -- use WD40 instead or, failing that, water applied from a hand spray. Even if the water doesn't lubricate the drill bit, it will at least help to keep it tolerably cool.

I must admit that, whilst I've not tried it as a drilling coolant or lubricant, I have used "I Can't Believe It's Not Butter" [1] when turning stainless steel; it seemed to work reasonably well, though the workshop stank like a chip shop for days afterwards.

[1] I'd bought two tubs in a B.O.G.O.F. supermarket promotion and, on tasting it, I soon decided I'd been overcharged on both. There again, I'd doubt that anyone could pay me enough to *eat* the stuff...

In article , Paul Hewish writes

IIRC, those "Piranha" drills are impossible to regrind to the same profile and may have too thick a web for a conventional re-grind.

formatting link
or, to download (18Mb),
formatting link

Except that, by then, the final hole may have wandered a little from where you'd like it to be.

The cutting point of a twist drill is meant to be the "chisel edge"; by drilling a pilot hole, you're making the drill cut on the flutes rather than the chisel edge and therefore the drill will faithfully follow the pilot hole. However, as the smaller drill is thinner, it is also more flexible and may have deformed or deflected as it was fed into the work- piece. Yes, it's a lot easier to drill one or more pilot holes, but it may not be as accurate as drilling with the "right" size of drill.

But then, if one really wanted accuracy, one would drill slightly undersize and then ream out the hole to the final diameter...

buy a pillar drill. Get some good quality metal drills, I bought a set from machine mart for about £30, sizes from 1mm to 13mm. Skimping on equipment will get you nowhere.