Takes time to skill up.

Likely lack of flux or it burnt off before. Also, the metal might not have heated high enough.

Think of a plummer sweating a joint - Torch is on the work to heat. Touch solder to joint and if it melts add just a little to fill the joint. If not hot enough, then continue adding heat and re-touching.

Martin

silver solder comes in all sorts of shapes etc jewlery silver solder i believe may contain fluirides that act as a very effective fluc--comes in different temperatuire ranges--talking here about jewlery grade

hth

I just recently did some silver soldering of stainless steel fittings to a pan stamped out of 16 gauge 304 stainless steel. I used Harris Safety-Silv 45 silver brazing alloy. See their website for details:

formatting link
. The reason why they call it Safety Silv is that it is cadmium free. Older silver solders contained cadmium, a toxic heavy metal like lead and mercury. I agree with Martin, it takes practice. The silver solder melts at

1300 degrees, so you really need to get the steel you are brazing a blood to cherry red hot. Without flux the silver solder wets very poorly. But with flux it wets like crazy to a wide variety of metals, making it very useful to join dissimilar metals. I used the black stainless steel flux made by Harris. Its a brown to black water based flux that you paint on well cleaned surfaces. At first the torch dries it out, then as the metal heats up, it melts. That is your first indication that you are getting hot enough to melt the silver solder. The problem is that the flux easily burns away if you overheat the metal. But if you control the heat, and get the metal hot enough the silver solder coats everything like crazy, its hard to stop it from flowing into crevices. Beware of the fumes from molten flux, they contain hydrogen fluoride gas. The cast iron table I was soldering on was corroded by the fumes. Another problem with silver soldering steel, and especially stainless steel is that you have to heat the metal above the transformation temperature. Now I only have a limited understanding of things like austenite and martensite, but basically if you heat steel above a certain temperature, you can dramatically change its hardness, toughness and other properties once it cools, often for the worse. With my stainless I found some corrosion around the soldered joints, and I am worried that chromium carbide crystals formed in the metal from heating it too long. Still, the joints are very strong.

I just unpacked a box that contained an old package - 1175 and 1300 - those were the part numbers - spec numbers - and the *F melting temps. The first was for non-ferrous or ferrous. The second was for Ferrous only - to high for coppers I guess.

The softness is also obvious - some are easily rolled and bent. Others are like steel wire almost.

In jewelery supply stores it is in flats, rounds, and wire formats. Even ball format.

Martin