I want to design a part using the same kind of metal - to - plastic interface as on the Krups 203-70 coffee bean grinders but I want to avoid the cracks in the corners.
If it gets posted it will be:
formatting link
Will this require say, a compliant adhesive gasket between my metal surface and the inside of the plastic reservoir or is this flaw primarily caused by a different problem, say a mixing issue that causes the plastic to be really brittle?
Thanks!
--Winston
Didn't find your answer? Ask the community — no account required.
Is "polish and coat with a hard brittle varnish" the answer to this question? ...
J
John R. Carroll
Those are stress cracks that result from the molding process, plasticizer migration and shrinkage over time. Thin walled parts are especially prone ti these over the lifecycle of the part. You also have to be careful when selecting a cleaning solvent (soap).
W
Winston
(...)
Thanks! This plastic stuff is complicated. Clearly I will have to turn that design task over to a specialist.
Apparently not too much time is required for the cracks to develop.
I shot the photo about 10 minutes after taking the grinder out of the box for the first time. I never even turned it on.
--Winston
J
John R. Carroll
I didn't realize it was new. Sheesh. The part has probably cracked at the knit lines. Poor knitting has a number of causes but chief among them is improper resin processing or low mold temperatures. IOW, somebody screwed up either when they designed the gates/runner system or when running the mold.
W
Winston
'Knit Lines'. That is a new one on me.
Ah Ha! So it passed final inspection while hot but grew the cracks in the Amazon warehouse? Wow!
Thanks again.
--Winston
S
Steve Ackman
Use a coffee grinder instead of a coffee basher? ;-)
L
Lloyd E. Sponenburgh
When I mounted splash shields on the table of my R2E4 (cast acrylic, and VERY prone to cracking and "spidering" from holes), I drilled the holes in the plastic to accept a grommet. IIRC, the holes were 7/16". I don't even want to have special bits around for plastics, so I drilled them way undersized, and used a tapered reamer to enlarge them without cracking the plastic.
The grommets were made for whatever hole size I drilled, and themselves had a bore of 1/4". The 1/4"-20 screws with a washer under the head fit just loosely in the grommets. When you squish 'em a little, the hole swells shut, and it holds firmly to both bolt and plastic, without any tendency for the plastic to be stressed at the union. Unless you use a shoulder bolt, you'll have to put a bit of threadlocker in the screw hole, since you cannot tighten the bolt too far without undoing the whole purpose of the exercise.
LLoyd
D
Doug White
"Lloyd E. Sponenburgh" wrote in news:Xns9E599A26A11FBlloydspmindspringcom@216.168.3.70:
Just make sure you keep the threadlocker AWAY from the plastic. I'm not sure about acrylic, but I know from sad experience what happens to Lexan when you get Loctite on it. We had a rush job that was just about finished when an overzealous technician decided to applied threadlocker to some 3/8" Lexan parts it took several days to machine. They swelled up & cracked like mad. Had to start all over again, with even less time.
Doug White
W
Winston
Help, Sir Coffee!
Is this one all right?
Can you recommend a better unit?
--Winston
W
Winston
So my intuition about an elastomer gasket wasn't too far off then, aye?
Excellent! Thanks Lloyd.
--Winston
W
Winston
Reminds me of a misadventure I had with acrylic and an acetone spill once.
Thanks for the reminder.
--Winston
D
Denis G.
It could be a material problem or maybe the part that broke was designed to use the minimum amount of plastic necessary in order to cut manufacturing costs. You could try your hand at plastic welding, maybe with a small soldering iron and proper tip. Another possibility might be solvent welding if it=92s made of PVC. I=92ll bet that the part wouldn=92t have broken if the sections were thick enough.
W
Winston
formatting link
formatting link
(....)
I'm not going to repair the existing grinder, especially since I need a different type anyway. (Who knew?)
My application will use softer plastic, so perhaps cracking won't be an issue.
--Winston
L
Lloyd E. Sponenburgh
Winston fired this volley in news: snipped-for-privacy@news2.newsguy.com:
Winston, you have mentioned the "other alternative".
Instead of holes, grommets, and bolts, some applications have a channel frame all-round the work with a u-channel-shaped gasket capturing the edge of the plastic sheet.
The only problem with this method for the 'ordinary' shop guy is getting gasket and frame material that will match up with one-another and the thickness of the plastic.
LLoyd
D
Denis G.
The only issue with a softer plastic might be a greater likihood of staining, but maybe it won't matter for your application.
W
Winston
(...)
You are right. This will be a 'liner' of a larger insulated container that will very rarely see the light of day.
--Winston
S
Snag
I like my B&D model CBM210 . I'm the only coffee drinker in my house . An
8 second grind makes just the right amount of coffee for my little 5 cup coffeemaker . I'm set like 4 or 5 clicks from the finest grind . And it's around 30 bucks at Walmart .
W
Winston
I had a very similar challenge sealing the end of a
30 gallon HDPE drum to the inside of a cylindrical plastic flange. The application did not require a lot of strength.
After I cleaned and degreased both pieces, I assembled them and flipped them 'opening down'. I poured some castable elastomer into the gap between the inside of the flange and the outside of the drum.
It worked a treat!
The elastomer was just 'runny' enough to find and seal the gap between the two cylinders, without leaking out of the gap. It was this stuff IIRC:
I expect that one could pour this stuff into a machined mold to create a gasket of just about any shape, too.
--Winston
W
Winston
(...)
Thanks, Snag!
--Winston
J
Joseph Gwinn
According to a Consumer Reports article some years ago, burr grinders work very well, especially for making a fine grind for expresso, but need a lot of cleaning to keep rancid coffee oil flavors.
We use a Krups Fast Touch Coffee Grinder, which is oval and of the impact type, and have not had problems with cracking. I recall that the broken grinder was not oval, and the cracks formed at the corners.
They retail for $13 to $18, so one does not repair them. Not that it's been needed, and the current one is at least ten years old.
Joe Gwinn
S
Steve Ackman
I haven't used that model, but I like the sound of the glass grinds catcher. It'd be a slam dunk if it had conical burrs. Google returns don't seem to include that model when "conical" is included in the search terms though. Even without the concial burr set... where else could you find a bright orange grinder?? ;-)
We have a Bodum Antigua conical burr grinder out in the trailer which, aside from the static around the plastic grinds catcher (only a problem in dry climes), has been fantastic for... oh, seven years or so. It was in daily use for espresso and drip for the first three years or so, then relegated to travel status when we got the professional-grade grinders.
formatting link
shows the Antigua partially dismantled. The second photo shows (a bit small) the upper and lower burrs. You can almost see how much cutting edge there is.
Conical burr grinders are generally considered better than flat burrs because they have much more cutting edge and can therefore be turned slower, creating less heat at the cut. They also tend to give a more consistent particle size. Flat burrs are generally less expensive and easier to replace. (For an almost comical description of how difficult one grinder is...
formatting link
)
Unfortunately, it seems the Antigua is no longer made. If I were looking in the sub-$100 range today, I'd certainly consider the Capresso Infinity. About $10 more than the grinder you're looking at, conical burr set... but plastic grinds catcher again. I don't know if this one has static problems or not... or if it does, how humidity dependent it is.
A review of the Infinity:
formatting link
HTH
Join the Discussion
Have something to add? Share your thoughts — no account required.
Didn't find your answer?
Ask the community — no account required
Report Content
You are reporting this content to the moderators. They will look at it
ASAP.