vertical up butt joint 3/8 or 10 mm

Dec 02, 2006 1 Replies
Jump to replies (1)

Problem with vertical up butt joint 3/8 or 10mm plate veed out to 60 degrees 2.5 root gap 2.0mm root face cannot get 100 percent penetration over 200mm what i need to know is what type of rods to use and the settings like the amount of amps will this be dc negative or dc positive



Stick or MIG , i have tried vert up and it dont work . The arc forces the fill out ,

Down weld forces the fill up and out , wider .. Looks like you milled it smooth on a mill ...

Penitation control is easiest with aws6011 , But 6013/7014/7024 need more current and flat .

I weld 6011 from Alloy Rods Corp at anywhere from 25 to 100 amps in 1/8" size .... 6013 needs at least 80 to 110 amps or the flux gets in the way ...

richbeav wrote:

Join the Discussion

Have something to add? Share your thoughts — no account required.

Didn't find your answer?

Ask the community — no account required