Basicaly, you need a diagram that shows stress vs. number of load changes. These diagrams distinguish between swelling and changing load. I don't know how you call them, but in German(y), the are called Woehler (or Wöhler)-diagrams. Might help you to google.
It is calculated this way:
f = F * l^3 / (3 * E * I)
f: deflection (in mm) F: Force (in Newton) 10N roughly are 1kg l: length (of the tube; in mm) E: elasticity modulus (in N / mm^2) it is (about) 0.7 * 10^5 N / mm^2 I: Umm, don't know how this translates. "Inertial moment"?
You get I with: (for a tube) I = pi / 64 * (D^4 - d^4)
pi: 3.14 :-)) D: outer diameter (in mm) d: inner diameter (in mm)
If (to explain the math) you take a tube with OD = 25mm, ID = 20mm and length = 1000mm you get:
Hope I didn't screw up the numbers, the calculater I had at hand was quite stupid. Don F. will jump in and correct me. I know. :-)
OK, deflection is very little, so will be the stress. If you want to know the stress, that's a different formula. Come back if you want.
Now the deflection is so little, that you will not have problems with stress, but only with fatique. I can't find that number right now, only for steel. And it is at about
2000000 ... 20000000 changes of load and reducing the allowable stress by about half. If you get more loads, it no longer matters. Now if I only could find: a) that limit-number of load changes. b) allowable stress with fatique.
But by guestimating, I'd like to say no problem with fatique. If your construction is critical, you need to investigate more on this and also need a certified engineer who is allowed do do the calculations in your state and will sign it.
HTH, for now, Nick
N
Nick Müller
That number is for alumin(i)um only. Just to put that straight.
Nick
N
Ned Simmons
Figure 5 in this paper displays the fatigue life of 6061-T6...
formatting link
I googled the search string: aluminum fatigue cycles 6061
Replace 6061 with your choice of materials - 7075 would be another candidate.
Ned Simmons
N
Nick Müller
Ah! That helps a lot. I don't have the time today to do the rest of the math, but I'll come back tomorrow.
Just a short addition to my other posting(s): Alumin(i)um continues to fatique with the number of cycles.
Nick
J
Jerry Martes
Hi Ned
Can 7075 *tubes* be obtained?
Jerry
N
Newshound
Once you have confirmed that the fatigue life is OK you have really got to think about fretting fatigue at the points where the tube is clamped and/or the load is applied. Aluminium is is a pig, especially for the home constructor. In my biker days I used to use Ally plate for fairing brackets usually clamped to the fibreglass with a sheet of rubber between, and they typically lasted 6 months.
N
Ned Simmons
Good question, Jerry. Based on the sort of thing 7075 is typically used for I assumed so, but have never personally had to shop for 7075 tubing. It appears to be available, but I'm sure it'll be quite a bit more expensive than 6061.
formatting link
Ned Simmons
J
Jerry Martes
Hi Ned
I rely on you and Don Foreman to supply the answers to questions I'm too dumb to be able to answer without studdying. I once worked with a smart guy who told me that 7075 was available in sheet *only*. I'm too lazy to reserch it so I'm depending on you guys who studdy to answer this 7075 tube question.
Jerry
W
wfhabicher
According to my ALCOA Aluminum Handbook (a little dated at 1957 copyright), 7075 T6 is indeed drawn into tubes.
Physical properties for 7075 T6: UTS- 83,000 PSI with extruded products having values 10% higher. YPS- 73,000 PSI with extruded products having values 10% higher. Elongation in 2 inches - 11%. Shear strength- 48,000 PSI. Endurance Limit (Fatigue Strength) - 23,000 PSI based on 500,000,000 (five hundred million!) cycles of completely reversed stress, using R.R. Moore type of (test) machine and specimen.
"These results are typical properties, average for various forms, sizes, and methods of manufacture and may not exactly describe any particular product." (quoted from handbook).
I must admit that I believed the endurance limit for aluminum to be much lower than this; but then it does not state the preparation of the test specimen such as surface finish, direction of lay of finish, shot peening, etc.
Wolfgang
Jerry Martes wrote:
J
Jerry Martes
Hi Wolfgang
Thanks for the correction of my misunderstanding that 7075 wasnt available in tube form. That 7075 is nice stuff.
Jerry
O
o.parafuso
I am carefully reading all your help, by the way, I deeply appreciate.
I can't understand a couple th------------------------
Of course, the result according to my calculations is 4.2Km J
I need help again.
I will come back with problems concerning the points where the forces are applied.
Martins
N
Nick Müller
That is the "force" (it ain't force, no nickpicking) of 5kg = 50N
No, 0.7 * 10^5. Thats 70000. You can understand that number like a spring rate. Quite a stiff spring out of solid.
0.7E5 is the engineering notation for 0.7 * 10^5. Maybe that confused you.
Huh!? I didn't write that.
f = F * l^3 / (3 * E * I) f = 50 * 1000^3 / (3 * 7000 * 11300) = 21 [mm]
Sorry, I misstyped something. Don't know where. Check that by yourself, I cant find my beloved pocket calculator and have to use the crap on the PC.
Checking the units: N * mm^3 / (N / mm^2 * mm^4) = N * mm^3 / (N * mm^2) = mm (looks good :-))
4.2 Km What is that? Did you mean 4.2 km? And J? Where do the Joule come from?
While I'm at it, I'll have a cup of coffe and calculate the stress:
s = M / W s: stress in [N/mm^2] M: moment in [Nmm] W: don't know how you call that (Resistance moment?) in [mm^3]
M = F * l F: Force (prev. posting) l: length (prev. posting)
W = pi / 32 * (D^4 - d^4) / D pi, D, d: prev. posting
Now with the real numbers (as I used in the prev. posting): W = 3.14 / 32 * (25^4 - 20^4) / 25 = 0.098 * 9225 = 905 [mm^3]
M = 1000 * 50 = 50000 [Nmm]
s = 50000 / 905 = 55 [N/mm^2]
Now I know that you don't want that. I'm sorry for my wrong guestimate in the previous posting, but 0.2mm deflection is quite different to the
21mm.
Now to the pdf about technical data Ned posted for the 6061-T6. Its elastic modulus (E) is 0.97E5. Quite different ('bout 30% off for the better) to the 0.7E5 that I assumed. Recalc with that number. You'll get a different deflection. The allowable stress for 6061-T6 is only 30N/mm^2 with just 1000 load cycles. **CRACK** With 10,000,000 (10Mio) about 15 N/mm^2 etc. see page 5, Fig 5. Thanks Ned for finding that.
An other comment from Newshound is also really important. The clamping. Your bar will break there. Don't use a tube at that place, but a solid. Make radii smooth and make a security factor of 2.
Remember that I still used that stupid calculator!
Nick
H
H. Martins
Sorry, but (I hope I am not wrong), f = 50 * 1000^3 / (3 * 7000 * 11300) = 210 !!!
The 'J' is just noise. I wrote a smilling face and something somewhere changed it to a 'J'.
I knew that, My point was that I according to my calculations, Elasticity calculations result should be 0.07 not 0.7E5.
Regards H. Martins (from correct e-mail now - the other was a browser mistake)
H
H. Martins
There is a mistake I previous post.
The Elasticity, according to my calculations, should be:
0.7*Force^5/length^2
0.7*50^5/1000^2 =218.75
... but you say it is 70000 !!
H. Martins
N
Nick Müller
Damned! My 7000 are a typo and really are 70000 as I initialy wrote. Now slowly:
f = 50 * 1000^3 / (3 * 70000 * 11300) f = 50 * 1,000,000,000 / 2373000000 = 21[mm]
Any zeros left out again?
The elasticity modulus (0.7E5) is a constant for the material. For
6061-T6 it is 0.97E5 according to the PDF. 0.7E5 is for "some" aluminium.
Where does that formula come from? What is Elasticity by your definition? Spring rate? There is a difference between spring rate (if you mean that by elasticity) and elasticity modulus. And in this case, it really matters. Maybe I confused you that you can look at the elasticity module as being a spring rate. It is, but only if you compress a solid bar and do not bend it.
Nick
N
Ned Simmons
I ran the numbers you used and came up with the same result.
1 m cantilever, 25 mm OD x 25 mm ID, 5 kg load applied at the end Deflection = 21 mm Max stress = 54 MPa
I don't trust the 97 GPa figure for elastic modulus - I used 69 GPa.
By the way, your "W" is "section modulus" in English, usually denoted "S".
Ned Simmons
N
Ned Simmons
I'm flattered you'd group me with Don, especially knowing that you're one of the folks here who limits his posts to those subjects on which you can speak with authority.
Not that I've noticed anyone posting riffs based on unfounded extrapolation and wild speculation.
Ned Simmons
H
H. Martins
Well, from your initial post:
You had wrote before:
I assume the above 'E' must be replaced by '(about) 0.7 * 10^5 N / mm^2' which you refer as elasticity modulus.
The 70000 figure seems do come from this formula, but a member of the formula is missing: 0.7*10^5 is indeed 70000, but we still have to divide by the square of the length which is 1 million. The result is
0=2E07. I am assuming " 0.7 * 10^5 N" is some sort of constant for this type of material.
Thanks H=2E- Martins
H
H. Martins
I suppose there is a typo:
1 m cantilever, 25 mm OD x 20 mm ID, 5 kg load applied at the end
Am I right?
H. Martins
H
H. Martins
Wait a bit, I didn't notice there were other posts. Let me read them all first.
HM
Join the Discussion
Have something to add? Share your thoughts — no account required.
Didn't find your answer?
Ask the community — no account required
Report Content
You are reporting this content to the moderators. They will look at it
ASAP.