A friend is making a copper weather vane. Basically a silhouette, but with 2 sides, each of which will have some 3 dimensionality. The 2 sides need to be joined at the edges.
He is talking about brazing, but I feel that for the effort & cost, it is overkill and soft solder would be adequate and sooo much easier. I'm pretty sure that he does not have an acetylene torch, or access to one. MAPP/propylene yes.
Suggestions?
Thanks, Bob
Didn't find your answer? Ask the community — no account required.
I think one of the phosphor copper brazing alloys will be as close as you'll...
M
Michael Koblic
FWIW:
If there are more than one joint I would avoid soft solder: The heating of the piece becomes critical and I have nearly lost my marbles while soldering one joint with the other joints coming apart simultaneously. There may be other issues with exposing soft-solder joints to weather.
I have had good success silver soldering using MAPP gas only with a Bernzomatic torch. I use the lowest melting point alloy.
J
Jim Wilkins
I've assembled durable 3D shapes in copper by folding a flange over for mechanical strength before soldering.
Depending on his soldering experience an iron may be easier to control than a flame. Once for fun I duplicated the TIG pattern of overlapping circles on the soldered seams around some RF filter cans by moving the iron back and forth and watching the puddle.
It's all practice. I have been at it so long I can splice 0.015" solder end to end into rings with an iron. Try it!
jsw
N
N Morrison
I'd tin the entire inside faces with solder, then sweat the edges together.
B
Bob Engelhardt
...
Wouldn't silver solder have the same problem with previous joints coming undone? Ideally you would have a progression of solders with decreasing melting points.
Well, they use soft solder on copper gutters, or don't they?
Thanks, Bob
M
Michael Koblic
Not in my experience. The heat conduction through copper is such that it is not difficult to achieve the 200-odd degC needed to melt the soft solder quite a distance away from the joint you are working on. It is much harder to do the same for a melting point of 600-odd degC. The heat tends to dissipate before it gets there unless the joints are *very* close together.
True, I think.
B
Bob Engelhardt
Just doubled thickness:
| | | | | | |||| ||||
or having overlapping edges:
| | | | | | ------ | ''''''''
or seams: | | |____ | ____| | | _____| |_____
How did you handle the problem of previous joints coming undone when soldering the next?
What size iron are we talking about here? I have a old iron that's just a 1 lb hunk of copper & is heated over a torch. Never used it - how would it compare to 'lectric?
I think that I'll need a little more practice first .
Thanks, Bob
B
Bob Engelhardt
Good point. That might help with something that he's worried about: keeping solder from where he doesn't want it. I.e., on the outside surfaces.
Thanks, Bob
B
Bob Engelhardt
OK, I can see that. But, talking about heat being dissipated, is it hard to get large pieces of copper hot enough for silver solder? Oh, I guess MAPP would do a much better job than propane.
Thanks again, Bob
L
Lloyd E. Sponenburgh
Bob Engelhardt fired this volley in news: snipped-for-privacy@news2.newsguy.com:
Bob, just as they say in the electronics trade, "Solder ain't glue".
Soft solder has virtually no tensile strenght, but is fairly strong in sheer. Hard solders are stronger, but still aren't intended to hold things together until after they cool completely; they are pretty weak when heated near-melting, but not quite.
Solder shouldn't provide the mechanical attachment; it strenghtens the joint, keeps it from moving after soldering, and keeps it sealed to the weather. The joint itself should be _mechanical_ in nature, and at least strongly-enough joined so that it will endure the forces of handing and fixturing during the soldering.
LLoyd
L
Lloyd E. Sponenburgh
Bob Engelhardt fired this volley in news: snipped-for-privacy@news2.newsguy.com:
Properly applied, the solder will form a meniscus between parts, and won't flow over the edges unless you apply too much.
You could apply a masking substance where you don't want it to migrate. I don't have any brand names at the tip of my tongue, but there are several for just that purpose. You might find them at a well-equipped art supplier.
Also, soft solder planes off any surface pretty easily with just a sharp knife. You could clean up any buggers fairly easily, then re- buff or re-texture the surface.
LLoyd
K
KD7HB
Propane is plenty hot enough for most silver solder on copper. Have to use plenty of flux to keep the copper from oxidizing while it is hot. The biggest problem with heating for silver solder is keeping the copper from walking away from the heat. Any sheet form will warp and twist from uneven heating. Need to clamp it quite well.
The lower heat from leaded solder will not warp near as much. Again, lots of flux!
Paul
R
rangerssuck
snipped-for-privacy@news2.newsguy.com:
Jus this afternoon, I was out in the garden and noticed that my wife had ponded some nails into a post and wrapped wire around them for a vine to climb on. I asked her about it, and she said she had done this a couple of years ago, with a roll of wire on my workbench.
It turns out that the wire was .020" flux core solder, and had been out in the elements for a couple of years, holding up a clematis with no ill effects. Given that bit of empirical data, I wouldn't hesitate to soft-solder a weathervane.
Also, if you apply the correct amount of heat, you really don't need to worry about adjacent joints. I, too, have amused myself by splicing solder. It's really not hard once you get the touch. .
A
AL A.
One commonly used masking substance (often called "anti-flux") is yellow ocher. You can get it from any of the jewelry supply places, on line or elsewhere. Jewelers use it for just that, to keep solders from flowing where you don't want them to flow. Just one such is here:
formatting link
Googling "yellow ocher" will find lots of others on the web as well.
For small stuff, I often use white-out, the correction fluid stuff. Works great. Just beware that some formulations (the non water based ones)of it are flammable and it makes nasty smelly and probably somewhat hazardous fumes when you first heat it. Take appropriate precautions and have good ventilation, etc.
As an aside, get yourself of a few of the jewelers supply catalogs. They have a whole world of cool neat-O tools, supplies, chemicals and gadgets, sure to fascinate most anyone who spends much time here...
-Al A.
L
Lloyd E. Sponenburgh
rangerssuck fired this volley in news:53f6b4ee-2729-4410-a26f-3ee0951c7a54 @k26g2000vbp.googlegroups.com:
hesitate
There's no question that soft solder will withstand the elements, but I'll bet dollars to doughnuts that the 20-thou. solder was not "holding up a clematis". Rather, it provided a growth path along which the clematis vines found their own purchases along the way. 60-
40 Kester .020 electronics solder has a tensile strength of about
10lb, when virgin and not corroded. Still... it would take quite a length of vine to equal 10lb, so it might have been holding it up, at least until it reached another catch point.
(pretty stuff, that, especially on a walk-under arbor)
LLoyd
D
dcaster
Propane is plenty hot enough, but large copper pieces do require thinking. I like to use IFB ( insulating firebrick ) to surround the work. If it is really big two or more hand held propane torches may be required. If it is not too big, I will first heat the part away from where I want to silver braze. So that that part is not sucking heat away from where I need the heat.
You might consider SilFos. It is copper with some silver ( up to
15% ) and some phosphorous which makes it self fluxing. But sometimes I still use some flux. Silfos is no good on steel, but is good for copper. Should be available at welding supply or plumbing supply places.
=20 Dan
M
Martin H. Eastburn
Go to a hardware store or a big box Home depot etc - buy some flat looking bronze - it is for plumbing - that of the air conditioning brazing. It is easily done with MAPP.
Mart> A friend is making a copper weather vane. Basically a silhouette, but
F
F. George McDuffee
======== I would suggest that this is not a new product/project as similar weather vanes have been around for 200 years or more.
Why not check and see how the people did it in the past as their techniques must have worked and lasted.
My guess would be a high tin soft solder and an organic flux with a big copper soldering iron. Most likely there were considerable mechanical joints/tabs/folds/rivets [and possible some wire lacing or stitching] and the solder was just used to seal things.
for some current production see
formatting link
old time
formatting link
There are many more sites.
Unka' George [George McDuffee]
------------------------------------------- He that will not apply new remedies, must expect new evils: for Time is the greatest innovator: and if Time, of course, alter things to the worse, and wisdom and counsel shall not alter them to the better, what shall be the end?
Francis Bacon (1561-1626), English philosopher, essayist, statesman. Essays, "Of Innovations" (1597-1625).
L
Lloyd E. Sponenburgh
F. George McDuffee fired this volley in news: snipped-for-privacy@4ax.com:
Um, Unk? When you make a post like that, you should suppress your sig line!
LLoyd
R
Richard J Kinch
This doesn't mean what it used to. Dunkin Donuts at the Florida Turnpike service plazas now charges $1 per donut. Parity has finally arrived.
J
Jim Wilkins
I made one piece larger and hammered a right angle flange, trimmed the flat edge on the other piece to fit inside it, then folded the flange over a little at a time. The problem is keeping the edges planar so they fit together after hammering the shape. I didn't get it right at first but was able to fold over the flange at the few places that met, then work around the edges to bring the rest in. The curved shape wasn't strong enough to withstand squeezing the pieces together with clamps. I think I used a piece of 1/4" steel upright in the vise for the anvil for outside curves and water pipe for the inside ones.
These days I have temperature controlled soldering irons, a nice one at work and an old Hakko without a readout at home. They are much nicer than uncontrolled ones because they can use a 2X - 3X more powerful heater without burning the tinning off the tip.
Previously I used a soldering gun or a 100W iron for larger jobs where a torch would cause damage, like melting wire insulation. If necessary I preheat the work on a hotplate or with a hot air gun.
The electric iron localizes the heat well enough to control the molten area. Solder changes appearance when it melts, less than steel but more than aluminum when TIG welding.
jsw
Join the Discussion
Have something to add? Share your thoughts — no account required.
Didn't find your answer?
Ask the community — no account required
Report Content
You are reporting this content to the moderators. They will look at it
ASAP.