I would like to know if welding aluminum is possible with a Millermatic 251, without a spool gun. That is, would the regular wirefeed be able to push aluminum wire through a regular MIG gun like Bernard Q-30 series. If so, what would be the typical grades of aluminum wire used and can I use 25/75 mix for that.
Thanks
Didn't find your answer? Ask the community — no account required.
Thanks Ernie,I was wondering about that - I'm looking at the Dimension...
P
Phil Kangas
a
regular
MIG gun like
grades of
Possible? Yes. Bitchy? Even more so. The only wire you'll push through that whip is the 5000 series. 4000 series is too soft to push. 5000 series is _very_ smoky and messy. You use straight Argon, and maybe a bit of Helium in the right circumstance. Would I do it? NFW! TIG rules, especially in repair work. YMMV phil
E
Ernie Leimkuhler
5356 wire, a teflon liner for the gun, pure argon or argon/helium mix. You have to keep the gun cable very straight, and clip off the wire flush with tip every time. For 3/64" wire use a 1/16" tip. Smooth drive rollers are best so you don't indent teeth into the wire, therefore increasing friction. Drive roller tension should be set so if the wire is stubbed out it slips on the drive rollers. This reduces the chance of bird-nesting.
One of the main problems is the slight delay in the gas flow. This will make a slight barf at the beginning of each weld, unless you hardwire an over-ride for the gas solenoid in the machine so you get pre-flow gas.
It can work, but it is a hassle.
D
David Billington
How common are rollers with teeth as I've only seen one, although I've only looked at a few dozen MIG wire feed rollers over 25 years. The particularly one was on a small low end MIG and was a PITA, as while I could adjust it to work OK and not birdnest at the slightest sign of the wire sticking, the owner couldn't. In the end just machined as much of the tops of the teeth out of the grooves to reduce the bite and job done, everyone happy.
I
Ignoramus15879
Ernie, thanks, it would seem that it is not worth doing that, right?
i
E
Ernie Leimkuhler
Depends... I did it for a project many years ago because it was my only option. It worked, but the first time I used a spoolgun I swore..."NEVER AGAIN".
You can rent a power supply for about $50 for a weekend, and a spoolgun to go with it for about $75. Plan your project to weld it over a weekend. It worked for me for years.
I know this sounds like sacrilege , but you don't have to OWN everything.
T
TinLizziedl
Gasp! ((shhh- don't tell Gunner))) ;>)
G
Gunner Asch
Ah...er....ahum......you dont? Really? Your kidding everyone...right?
No?
Damn
Sigh
Gunner
"Lenin called them "useful idiots," those people living in liberal democracies who by giving moral and material support to a totalitarian ideology in effect were braiding the rope that would hang them. Why people who enjoyed freedom and prosperity worked passionately to destroy both is a fascinating question, one still with us today. Now the useful idiots can be found in the chorus of appeasement, reflexive anti-Americanism, and sentimental idealism trying to inhibit the necessary responses to another freedom-hating ideology, radical Islam"
Bruce C. Thornton, a professor of Classics at American University of Cal State Fresno
Join the Discussion
Have something to add? Share your thoughts — no account required.
Didn't find your answer?
Ask the community — no account required
Report Content
You are reporting this content to the moderators. They will look at it
ASAP.