I'm a carpenter and I used to get my gate frames made by a friend who has moved away, so I decided that I would make them myself. I've had an arc welder for a while and while I'm no expert I'm reasonably competent with it. The problem I'm having is that when I try to weld 25 x
25 x 1.6mm square tube I sometimes blow holes in it. My solution has been to use 2.5mm tube, but this is more expensive and not really necessary for the application, so I'd like some information (Advice, Links etc) on how to successfully weld the lighter gauge steel. I'm using general purpose 2mm rods, and my welder doesn't have an amp scale but has a gauge to match rods with material and I've experimented with a lot of amperage settings but can't seem to get a good clean weld on the thinner stuff. I have no problems with heavier stock. Any help greatly appreciated. Neil.
Didn't find your answer? Ask the community — no account required.
Randy, I tried grinding a vee on the "outside of the bend" and rewelding. That...
R
RoyJ
1.6mm is 16 ga (.062") on this side of the pond. I'm assuming you are trying to weld an end of one tube to the side of another tube. This is relatively thin tube, you will always have trouble with the end cross section burning away on you.
A few suggestions: joint prep is critical. Since you aren't an expert welder, spend your time on the prep. The joints should have no gaps, the cuts should be square, there should be no sharp edges that will melt too quickly. Use 6013 rod (not sure if you can get that exact variety). It is designed for thin material, minimal penetration, easy slag removal. Experiment with the amperage selection. There is a setting that will give you the best compromise between the penetration you need for strength and the excess heat that blows holes. The exact setting is very much a function of the specific welder used and the specific weldor skills.
OK, the punch line: PRACTICE!!!
Cheers.
Neil Green wrote:
G
Grant Erwin
You are essentially trying to stick weld sheet metal, which is a chancy proposal at best. This is a really good reason to upgrade to a MIG welder - there you can just look up the setting for 16 ga. and weld all day long.
You can run stick a lot cooler if you try running it with the polarity reversed from the way it normally is. Try running DCEN instead of DCEP, that may help. There's some rod that this works very well with, but I can't remember it offhand, nor do I do this dodge myself, having other options.
Grant
R
RoyJ
Sheesh! Why not just suggest getting a TIG welder? (Sarcasm!) I can teach most anyone with a steady hand and a willingness to learn and practice how to stick weld this project in 4 working hours (spread over several days) Clean metal, good fitup, proper rod, downhand welding, and a buzzbox with reasonable OCV and you can easily match a MIG weld. OK, I'll grant that you will have more spatter to deal with.
The 16 ga 1: tube the > Neil Green wrote:
B
Bob Engelhardt
This sounds like the frames are for professional work that you do. In which case it's worth it to have it done right. You will never get it done right with your stick welder and being "reasonably competent". Finishing a whole gate without burn throughs will be impossible. Burn throughs are ugly and would give the whole gate an unprofessional look.
I've 2 suggestions:
Get a small MIG & learn how to use it(!), or
Pay someone to do the welding. This might be done pretty cheaply if you do all the cutting/fitting and take it to him all jigged up, so he only has to weld.
My $.02, Bob
N
Neil Green
Thanks for the advice Roy. I have a cutoff saw so the cuts are square, I guess it is just a matter of practice. The rods you suggested are 2.5mm from what I've been able to discover. I have some of these but I've been using 2.0mm. Would I be better to use the bigger rods? Also, are any particular type of rod better for this work than others? The type I have are general purpose, I bought them from an engineering supply so I presume they are of acceptable quality. Thanks for your help. Neil.
N
Neil Green
Thanks Bob, but the main disadvantage to having someone weld the frames is that by the time I cut them, take them somewhere to be welded then go back the next day to pick up the finished job it wouldn't pay as far as my time is concerned. When my friend lived close by this wasn't an issue. As I said I have no trouble using 2.5mm square tube but it's more expensive and not necessary for structural integrity. I'm fairly sure that the 1.6mm material can be successfully welded with a stick welder, I just have to learn how.
G
glyford
6013 is the type, not the size, they come in many sizes. It should be available in 5/64th (2mm). You may even find it in 1.5mm (1/16th). That said, you may find the 2.5mm will work just fine--I've found the smaller rods can actually be harder to control, sometimes. You may also want to try the 7014 type rods.
If it's a better type for the work you're doing, sometimes the size doesn't matter as much. If you already have some on hand, it's worth trying. Start with the amperage selection listed on the package and go from there. --Glenn Lyford
R
RoyJ
As glyford mentioned, 6013 is the type or spec on the rod, not the size.
formatting link
You don't mention where you are at so I'm not sure how that will translate to local suppliers. The 6013 has a very soft arc, is not at all aggresive in 'dig' or penetration. It was original developed for thin sheet metal applications. When properly done it leaves a nice soft slag that sits on top of the weld.
formatting link
out page 16 of the catalog and bring it to your welding supplies dealer.
I'd be concerned with your "general purpose" rod. The other common rod (read CHEAP!) rod is 6011 which is good for rusty or poorly cleaned metal and has the necessary 'dig' to get through the rust. This rod will burn through like you have been noticing. You could try a test: run a nice bead on the side of a piece of scrap tube. Try for a very even, almost fat bead. After it cools, examine the slag. If the slag is dark, a bit porous, and completely covers the weld area, and chips off with one tap of the hammer, it is likely 6013. If it is glassy or shiny, does not cover all the weld area, and has to be tapped several times to remove, it is likely 6011.
When you weld an end to an edge, focus the rod more to the side of the long tube and away from the edge end of the other tube. If you have a weld that involves one end out in the air, start on that end (on a gate that usually means weld form the outside to inside) since the coldest part of the weld is at the start. Try to weld everything downhand. Run your current as low as possible consistent with keeping a clean arc. Keep the arc short.
Practice Practice Practice! Figure it will take several total hours of practice over several days or a couple of weeks to master the eye hand coord>>1.6mm is 16 ga (.062") on this side of the pond. I'm
P
Pete C.
I'd agree. Stick seems more suited to heavy structural welding than light tube frame work though I'm sure the pros can do it. I'm not pro, but frequently my welding projects are made with 16ga square tube in
1/2" - 1 1/2" sizes. I TIG weld it and rarely have any problems.
Pete C.
R
Richard Smith
Would welding vertical-down help Neil?
I've no experience of stick welding this thin. I know 6010/6011 and
6013 vertical down works for thinner stuff.
Richard Smith
J
JohnM
As has been suggested, try a 7014. It's very forgiving and tends to look good even if you didn't run a perfect bead.
Run hot and fast. Traveling slowly causes the heat to spread along the surface of the metal, that's where you get the big holes when the puddle falls through. Keep a short arc, just as short as you can, and know what you're going to do before you do it. Lean on something so you're as stable as possible and turn the work so it fits your natural motion.
You should be able to run this weld with a 6011 too, try it on AC. Try the 7014 on AC too..
And keep at it, you'll get it.
John
B
Barry Lennox
It's not so easy (at least for me) I built a light trailer frame from
25 x 25 x 1.5 mm and had the same problems you outline. What eventually helped was 2mm 7014 rod, a short arc and a fairly high feed rate. But most important was about 2 hours of practice spread over the best part of a couple of days.
Best of luck (but practice will be better than luck !!)
Barry
J
John
I've seen my dad weld on thin tubing and other thin metals before with a stick welder. Just get a few pieces and practice till your comfortable with your welds.
S
Steve B
"Neil Green" wrote
I was a steel erection contractor for nine years. In that time, I repaired a lot of thin walled tubing on gates and fences. I used 6011 3/32" rod exclusively, BUT, used it against suggestions with electrode NEGATIVE. If you can dial down your welder, you can run it, but it takes time getting that fine touch required to carry a small puddle, or "stack dimes" with a whipping action.
Since you're in another part of the world, I don't know what the conversion factors would be, but you should be able to find those out easy enough.
For a pound of rods, try it. It might just work for you.
Steve
N
Neil Green
"Neil Green" wrote in message news:46708d7b$0$994$ snipped-for-privacy@news.optusnet.com.au...
Thanks to everyone for the expert and practical advice, a very helpful group. I'll score some of the rods recommended and give them a go. Thanks again. Neil.
J
Jimmie D
I was having a similar problem repairing my daughters trampoline. The metal is very thin and I was burning through using an E6011. Change to an 6013 and no problems.
S
Steve B
"Whether you think you can or can't, you're right."
Henry Ford
E
eviltexan
I was buildin a fence and gate for an apartment complex with my job. Trust me I know what you are goin thru, my boss showed me the trick for it though and it works like a freakin charm. What you do is turn your amperage down a bit and make a series of tack welds. Just one after another, kinda overlapping them. Make SURE you do it to where they are GOOD penetrated tacks, but dont stay on there long at all. After you have done this across the joint you are welding, crank up the amperage then go back and make a good strong weld over the tacks. What thats gonna do is melt all the material in together and you should have a good strong weld without having punched thru the metal. This works, trust me, my boss didnt believe in mig welding in the field, all we burned was the big Miller Gas engine welders and 6011 rods. It will do the trick for you. We built fences, gates, handrails. Hell we did it all with stic welding. Good luck bud.
S
SteveB
As I have previously stated many times, DC stinger negative with 3/32" 6011 rods, and weld like you're stacking dimes. Works like a charm. Make your amperage just high enough to run.
Steve
Join the Discussion
Have something to add? Share your thoughts — no account required.
Didn't find your answer?
Ask the community — no account required
Report Content
You are reporting this content to the moderators. They will look at it
ASAP.