Hello,
Does anyone knows thermal expansion properties according whith température of 304L Thank you
Pierre
Hello,
Does anyone knows thermal expansion properties according whith température of 304L Thank you
Pierre
Google should know.
Michael Dahms
Approximately 9.6 X10 E-6 per degree F.
304L stainless steel has a CTE of
16.9 x 10^-6 / degree C (RT - 100C) 17.3 x 10^-6 / degree C (RT - 300C) 18.4 x 10^-6 / degree C (RT - 500C) 18.7 x 10^-6 / degree C (RT - 650C)