A350 and super duplex

Oct 20, 2006 3 Replies
Jump to replies (3)

I have been offered needle valves with A350 body, for OS&Y bolting, supplier suggests super duplex bolts instead of L7.



Will it represent galvanic corrosion problems ?



Thank you,



These are 1" needle valve, A350 LF2 body

IMHO, minor - the super duplex needle stem is cathodic with respect to the A350 valve body (anode) - the valve body has the larger surface area - same area effect as seen in the use of brass valves in domestic water service with A53 steel pipes. BTW - the properties of the fluid that valve control will constitute the dominate corrosion mechanism(s).

Ed Vojcak