I wanted to create very light hollow metal ornaments that could float by the buoyancy of the air inside. I wanted to use metal because some parts of the object would need to withstand an ambient temperature of about 100-150 degrees celsius. I figured a good thickness for the metal would be about 0.5 mm, enough to withstand moderate handling without deforming. I'm not a craft expert, but I the best idea I thought of would be to do the following:


1) create a master object from clay or polyclay
2) use the master to create a mould from plaster
3) use the plaster mould to make a wax copy of the object
4) apply an initial film of nickel by solution or aerosol spray
5) plated the metal of choice onto the nickel to the desired thickness
6) immerse the object in boiled water to melt the wax
7) wax can then be skimmed off and recycled

The object shape could be quite complex, for example a flower with petals or miniture scene with a house or something. I might end up producing small batches of a 1000 or more. Can anyone comment on my proposed technique? Would there be a better or simpler way to do it? How would an industrial production line do something like this? I realise I can enlist the services of metal plating companies to deal with some of the work. Comments please.



Many thanks, Erik


low cost method:

  • for hollow metal shapes
  • take a heavy block of wood, akin to an old tree stump,
  • carve out a negative shape of your object,
  • take thin sheet metal,
*hammer out shape into wood block.

go visit a local custom jewelry maker for ideas or contract the work out

if very complex shape make wax mould and have parts cast out of your desired metal via "lost wax"

Little more expensive method:

  • make your design in CAD
  • go to tool and die shop
  • make set of dies
  • punch out product

If the shape is very intricate with a lot of relief you would probably be better off casting the piece

snipped-for-privacy@psydolphin.net (Marin) wrote in news: snipped-for-privacy@posting.google.com:

If you want them to float in water, then you will need them to be completely sealed. This is going to be difficult, since relief holes are needed during the casting and cleanup process. Plan on sealing up some holes as part of your manufacturing process.

There are many plastics that can withstand those temperatures.

Easiest would be plastic injection molding. Next best would be lost wax casting.

Not hard to do. Make up stamping molds for two or more sides as needed and use brass as the metal (easily soldered without problems) and solder the parts together. Don't forget to have a vent hole which gets sealed after the soldering of the parts together and everything has cooled otherwise you won't be able to get a seal with the soldering process as there will be a good vacuum inside.

-- Bob May Losing weight is easy! If you ever want to lose weight, eat and drink less. Works every time it is tried!

The process you're talking about is called electroforming. A nonconductive master is painted with a conductive paint and a layer of metal is electroplated over it.

Properly done the metal reached a thickness sufficient to support itself and can be removed from the master.

The "good" surface of the piece is usually the side that faces the mold, the side toward the solution comes out all knobby.

While it could be done on a shoestring, it requires more equipment than a couple of drycell batteries and more know-how than a little bit.

I would suggest, if you're not already well versed in electroplating, that you job it out.