Anodizzare l'alluminio

Jan 24, 2007 3 Replies

Una volta avevo letto una pagina web che spiegava il metodo casalingo per effettuare processo in oggetto. Qualcuno ne sa qualcosa? Non trovo più le info necesarie...



Ciao,

A discussion on news:uk.rec.models.engineering , via

formatting link
formatting link
There's also blu_swede's/Scott Peterson's method:
formatting link
"Home anodizing files"

formatting link
formatting link
Vriendelijke groeten ;-) Ron van Sommeren

14th.int. electric fly-in, Aug.26, Nijmegen, Netherlands
formatting link

-------------------------------------------------------------------------------- I am using the free version of SPAMfighter for private users. It has removed 39 spam emails to date. Paying users do not have this message in their emails. Try SPAMfighter for free now!

Ciao,

formatting link
Colouring and protecting IRON:
formatting link
Materials and manuals:
formatting link
Below the description of a method by colleague 'Aerobscure' from France.

---------------

The process described s a not hard anodizing but decorative.

Anodizing aluminium is easy but the simplest way doesn't works with all the aluminium alloys. You will have bad results with 2017 and 2024 (dural) excepted with very dark colors. It works well with the 5xxx, 6xxx and 7xxx serie.

The steps are :

1- degreasing the aluminium parts

2- Anodizing.

For this operation you need a non conductive tank (pyrex is well) and a power source about 15 V (a 12V car battery is fine, it's a 13,8 V one !); the solution in the tank is 80% distilled water and 20% sulfuric acide. Connect the anode (+) to the aluminium part and the cathode (-) to a large sheet of lead (with gloves please !); The density of the current will be a bout 1A to 2A dm2. You can use a variable resistor for the regulation or some car light bubbles. Let in the bath for 30-40 mn. After that you will rince the part with water and a basic solution (ammoniac, soda ash, Deskstop ...)

3 - Coloring

The most findable coloring agent in France is used for clothes under the brand name DYLON. It's a powder you add to boiling water. Immediatly after anodizing put the aluminium part in the colored boiling water during 2 or 3 minutes. Dry it and repeat until you find the best coloration.

We have opened the alumine cells by anodizing, colored them and we must closed the cells. There is different solutions.

- Hot water just before boiling (

Ciao,

You could contact Maurizio Martinucci

formatting link
motori brushless

-> particolari in ergal anodizzato.

Or Massimo Ferraresso

formatting link
Vriendelijke groeten ;-) Ron van Sommeren

14th.int. electric fly-in, Aug.26, Nijmegen, Netherlands
formatting link

-------------------------------------------------------------------------------- I am using the free version of SPAMfighter for private users. It has removed 39 spam emails to date. Paying users do not have this message in their emails. Try SPAMfighter for free now!