Why would the exact same spot fail four prints in a row?

Nov 19, 2026 Last reply: 2 days ago 5 Replies

First reply

maple_knot

Before anything else: hollow the model out if it isn't already. A solid print puts all the pull from every single layer on one concentrated spot on the FEP, and that can do real damage to the film as well as cause the print to fail. That's the first thing I'd fix regardless of…

Read the full reply

Something wierd is going on with my Saturn 4 Ultra and I've run out of ideas. Two years of flawless prints, and now this one 'happy couple' model keeps failing. Four attempts, all four botched in basially the same place, and it's always just the guy. The woman comes out perfect every single time. The failure shows up as horizontal gaps through his head and jaw, plus some lifting near the collar.



My setup: updated SatelLite slicer, Elegoo's ABS-like 3.0 Pro, bottom exposure of 30 seconds over 5 layers with 5 transition layers, 2.8 second normal exposure, 1.0 second wait before cure, resin started at 25°C.



Here's what I've already done. Re-ran ResinXP2 and the V3_cones test, results match the settings above. Used the printer's built-in UV uniformity and flatness check, all good. Gone through the problem area layer by layer in SatelLite and UVtools, no voids, nothing odd. I even joked about putting garlic and candles around the machine in case some ghost objects to this particular couple getting duplicated. As I type this, a fifth attempt is running with the model rotated 90 degrees, backs facing down. Is there anything else I should be checking? At this point I'll take any theory, no matter how strange.


Before anything else: hollow the model out if it isn't already. A solid print puts all the pull from every single layer on one concentrated spot on the FEP, and that can do real damage to the film as well as cause the print to fail. That's the first thing I'd fix regardless of anything else, because even if you solve this particular failure, running solid models repeatedly is asking for a torn FEP down the line.

And that leads me to my second thought, which is the FEP itself. Two years of service is a good long run for that film, and if this model has indeed been printing solid all this time, the film may already be stretched, scratched, or clouded in the area where the male figure sits. Consider replacing it. It's cheap, it's quick to swap, and a worn film changes how the print releases layer by layer, which can absolutely produce failures that cluster in one part of one model while the rest of the plate comes out fine. The way you describe it, the man and woman print side by side on the same plate with the same exposure, same resin, same everything, and only the man fails in the same spot every time. That points away from the printer and toward the model geometry. The diagnostic work you've done is thorough, but if the male figure is heavier and bulkier than the female, every cured layer of him pulls that much harder during release, and any weak point in his head and jaw will show it first.

If it turns out the model is already hollow, then check that the drain holes are actually open and placed at the bottom in your current orientation, because trapped curing resin inside a hollow model behaves a lot like a solid one. Either way, a fresh FEP plus a properly hollowed model with good drains is where I'd put my money before chasing anything spookier than that.

Reading this made me think of the way you described the guy failing in the same spot every time. If the fifth attempt with him turned on his back still shows those gaps through the head, does that change anything about the pull force idea? I only ask because I just started with my own little figures and I'm still learning what all the settings even mean. The part about the stretchy film under the build plate makes sense to me, since two years feels like a long time for anything in this hobby. Keep us posted on how attempt number five turns out, I'm genuinely curious now.

I keep seeing this blamed on the film being worn out, and I have to push back a little. If the release surface in that one spot was stretched or cloudy, it should mess with everything on that side of the plate, not just one figure. The woman prints right beside him every time and comes out clean, so the film is clearly releasing fine where it matters. To me that points back at the guy himself, the geometry around the head and jaw, maybe how the supports are placed in that area. What does the support density look like on his head compared to hers, and are the tips thin enough that they could be snapping mid print?

That garlic and candle joke hits home, we used to blame gremlins for everything back before we had forums to argue in. Old habits die hard but your layer-by-layer checks are the modern version of squinting at a print under a lamp, and they still hold up. One thing I keep coming back to: you said the wait before cure is short at 1.0 second. On some machines a touch more dwell before the plate lifts lets thicker sections settle, and a bulky head is exactly where that shows. Might be worth a try alongside the rotation you're alredy testing. Did the fifth attempt come out any better with him on his back?

The detail about the wait before cure caught my eye too, and I want to restate it carefully, because there is a difference between the dwell time after the plate lifts and the wait before the light actually fires. You listed 1.0 second wait-before-cure on top of a 2.8 second normal exposure, which is on the brisk side from what you describe, and a heavy cross-section like a seated figure with a table and base can still be moving slightly when the next layer cures. If the fifth attempt on his back still gaps in the head and jaw, that would strengthen the case that release force at the man's bulkier upper half is the culprit rather than anything in the slicer.