you will find Johnson Matthey's publicity blurb for their brazes and silver solders. On p 11 you will find that that their 56% silver solders have a tensile strength of 410 n/mm^2, or 60,000 psi.
There is also a 44% alloy with a tensile strength of 545 N/mm^2, or
80,000 psi. It's a bit harder to use though.
Or here, where the UTS of a 56% silver solder is given as 71,000 psi:
formatting link
56% silver solder is strong stuff. UTS varies between about 50 ksi for cheap stuff to 70 ksi plus for the good stuff. Yield strengths of 60 ksi are not uncommon for premier brands.
Ans yes, joint strengths can be higher, up to maybe 120 ksi.
-- Peter Fairbrother
Didn't find your answer? Ask the community — no account required.
While you're at Home Depot for the roof patch....
P
Peter Fairbrother
If "over here" is in the UK or EU I can perhaps put you onto a supply of "real" MAPP gas. Might need a different torch or an adapter, it has en412 (I think that's what it's called, used on butane torches and camping stuff) threads.
There is also the MAP_PRO type of gas (propylene, comes under several other names apart from MAP:PRO), but that is fairly easily available, most plumbing supply shops carry it.
(Technically MAPP is a tradename, but the people who own the name stopped making it about five years ago. People like Rothenburger and Benzomatic started selling propylene under names like MAP:PRO and MAP:PLUS instead, as a substitute.
However "real" generic MAPP gas was/is methylacetylene/propadiene mix stabilised with propane or more likely commercial propane/butane mix. while MAP:PRO and the like are pure-ish propylene.
MAPP is better, especially for welding - you can just about weld with oxy/MAPP, but forget about it with oxy/MAP:PRO.
However for air-gas torches, the difference is less important, and air/MAP:PRO is usefully hotter then air/propane. )
-- Peter Fairbrother
P
Peter Fairbrother
Harris Stay-Silv 56 does not contain added phosphorus. There are grades of Stay-Silv which do, but not the 56% grade, which is specified by Harris as being particularly good for nickel alloys and stainless (and no mention of copper pipes).
-- Peter Fairbrother
J
Jim Wilkins
Pure iron 4,000 PSI:
formatting link
What is your point?
S
Stumpy
propane is hot enough, but on larger items can not supply heat fast enough. Erik has some good suggestions about using insulating fire brick to contain the heat. I have used more than one small propane torch to heat things faster.
Dan
-----------------------------------------
I did make a mental note about his suggestion. The welding shop doesn't have fire brick or glass wool, but I'm keeping my eyes open.
Waiting on parts anyway, so no hurry.
S
Stumpy
I picked up some Radnor Safety-Silv 56, it must be a subsidiary of Harris Products.
E
etpm
No I'm not. I was commenting on the strength of the solder itself independent of joint design. Joint design can indeed lead to an even stronger assembly than the tensile strength of the solder itself would suggest. Bad joint design can lead to a weaker assembly too. Eric
E
etpm
I was originally talking about Harris Saftey Silv. Not Stay Silv. I think the reason it is called Safety Silv is because it contains no cadmium. Anyway, it is good for steel. Eric
S
Stumpy
Would pink insulation make a good shoebox sized brazing grotto?
formatting link
"The Complete Metalsmith" is in transit.
E
etpm
I don't think pink insulation, or any type of home fiberglass insulation will work. I think they use some kind of binder that you probably don't want to breathe when it outgasses from the heat. Where are you located? Anywhere near Seattle? Eric
S
Stumpy
Ha, Not very close.
I'll find a local source. Ebay and Amazon charge as much for shipping as they do for the bricks.
I'd prefer glass wool because I could stick it in a jar to save for future projects. I wonder if 1/2 oz is enough to accomplish anything.
formatting link
J
John B.
Nope. Over here" is Thailand but probably covers Malaysia and Singapore also as I have enquired in a number of places and "no have".
J
John B.
I don't see any "Stay-Silv 56" listed in the Harris catalog and all the "Stay-Silv" I see listed does contain phosphorous. There is a "Safety-Silv 56" though.
formatting link
J
John B.
Radnor is made by Harris and is (I think) a name for their flux coated rod.
J
John B.
Yes, Safety-Silv does not contain cadmium and yes it is good for steel. I was responding to the O.P.'s reference to "Lincoln Stay-Silv".
D
dcaster
Pottery supply places and foundry suppliers. Seattle Pottery on the West Coast. Sheffield Pottery Ceramic Supply East Coast.
Dan
D
dcaster
Try the gardening supply for Vermiculite and perlite. Building supply for Rock wool. Not glass wool.
Dan
M
Martin Eastburn
I finally was able to get the pdf mentioned below.
formatting link
The %2520 is a double space concept but only singles work out. Might be due to a foreign font used.
Mart> >> On Tue, 05 Feb 2013 08:59:41 -0800, snipped-for-privacy@whidbey.com wrote: >>
formatting link
formatting link
P
Peter Fairbrother
formatting link
I dunno, works fine for me.
But try:
formatting link
76,000 psi Tensile
60,000 psi Yield
or just google something like "silver 56% tensile" and look for the manufacturer's hits. It shouldn't take long to convince you that 70 ksi UTS, 60 ksi yield is fairly typical for a good 56% silver brazing alloy.
Lots of people find it surprising, but it's so.
-- Peter Fairbrother
S
Stumpy
Hey Eric,
I got the job done. The low temperature propane brazing didn't work for me. I just got a ball of solder sitting there - it never went into the joint. Luckily I had the O/A setup available - instant success.
I like brazing. It's a very strong joint and I only used about 1.5" of the S-S56 rods and I still glopped on too much.
The rest of the assembly was torturous. 18 pages of text could have been replaced with 3 pages of diagrams.
Join the Discussion
Have something to add? Share your thoughts — no account required.
Didn't find your answer?
Ask the community — no account required
Report Content
You are reporting this content to the moderators. They will look at it
ASAP.